Welding gas chart: the right gas for the metal, by thickness
The trade default, in one line
For mild-steel MIG work, an argon/CO₂ 82/18 or 80/20 mix is the working default. Clean bead, manageable spatter, fair cost per cubic metre. If a workshop only runs one cylinder, that’s the one.
For TIG on anything, use pure argon (welding-grade 99.997%, or 5.0 where precision matters). That covers most of the work most shops do.
Everything below shows what to change when the default isn’t right.
Mild steel — MIG
| Thickness | Shielding gas | Purity | Typical flow | Notes |
|---|---|---|---|---|
| ≤1.6mm | Ar/CO₂ 82/18 | 99.997% | 12–15 L/min | Thin section, prone to burn-through. Keep travel speed up. |
| 1.6–3mm | Ar/CO₂ 82/18 | 99.997% | 13–16 L/min | Sweet spot for the default mix. |
| 3–6mm | Ar/CO₂ 80/20 | 99.997% | 15–18 L/min | Slightly hotter arc. Can also use 82/18 at higher amps. |
| 6–10mm | Ar/CO₂ 75/25 | 99.997% | 17–20 L/min | Deeper penetration. Multi-pass likely. |
| >10mm | Pure CO₂ or Ar/CO₂ 75/25 | 99.5% / 99.997% | 18–22 L/min | Pure CO₂ wins on penetration; trade clean bead for fusion. |
Pure CO₂ is cheap and runs hot. Fine for structural and hidden welds; less ideal where finish matters.
Mild steel — flux-core (FCAW)
Two flavours, different rules:
- Self-shielded (FCAW-S) — no gas. The flux does the whole job. Good for windy sites.
- Gas-shielded (FCAW-G) — run 100% CO₂ or Ar/CO₂ 75/25. Higher deposition than solid-wire MIG, useful on heavy structural.
Stainless steel — MIG
Pure argon doesn’t work for stainless MIG — the arc is cold and unstable. You need a small active component to stabilise it.
| Thickness | Shielding gas | Notes |
|---|---|---|
| ≤3mm | Tri-mix (Ar 90 / He 7.5 / CO₂ 2.5) | Best bead profile, low carbon pickup. |
| ≤3mm budget | Ar/O₂ 98/2 | Cheaper. Slightly harsher arc. Fine for non-cosmetic work. |
| 3–6mm | Tri-mix | Hotter arc from helium helps on thicker sections. |
| >6mm | Tri-mix or Ar/O₂/CO₂ custom blend | Call for a mix matched to your wire — we’ll size it. |
Stainless steel — TIG
Pure argon 5.0 (99.999%). Add a backing gas (also pure argon) for full-pen root passes on pipe — contamination of the back side will ruin the weld.
Aluminium
| Process | Thickness | Gas | Notes |
|---|---|---|---|
| MIG | ≤6mm | Pure argon | Welding grade 99.997% is fine. |
| MIG | 6–12mm | Ar/He 75/25 | Helium adds heat, speeds travel. |
| MIG | >12mm | Ar/He 50/50 | Preheat may still be needed. |
| TIG | Any | Pure argon 5.0 | Period. Never compromise. |
Reactive metals (titanium, zirconium)
Argon 5.0 at minimum, and purge the back side. Consider a purge chamber for critical welds. These metals will react with any residual atmosphere at welding temperature.
Flow-rate and draft rules of thumb
- Indoor still air — around 12–18 L/min for most MIG work. Too high and you introduce turbulence which pulls atmosphere into the weld pool.
- Windy or outdoor — push to 20+ L/min and consider a wind break. Once wind exceeds 8 km/h, gas shielding gets compromised; either move indoors or switch to flux-core.
- TIG — 10–15 L/min is enough. Higher flow doesn’t help and wastes gas.
Cylinder-size rules of thumb
| Use case | Recommended size |
|---|---|
| Occasional MIG, single welder | E-size |
| Full-time single welder | G-size |
| Two or more welders daily | Multiple G-size cylinders |
| Portable site rigs | D or C-size |
| High-volume TIG shop | High-volume argon supply setup |
Draw rate matters more than absolute gas volume. If you’re emptying a G every day, it’s worth reviewing a higher-volume supply setup.
Cylinder-size rules of thumb
MIG and flux-core dominate the volume in most fabrication shops because the travel speed is high and training time is low. TIG is slower but produces the cleanest bead profile, which is why it rules in stainless food-grade work, aerospace, and the kind of visible welds that never get ground back.
The gas decision follows the process, not the other way around. If you’re setting up a new rig, decide the process first, then pick the gas, then size the cylinder.
Cylinder-size rules of thumb
Solid wire (ER70S-6 for mild steel) works well with the standard Ar/CO₂ mixes. Metal-cored wires often push better with slightly higher-argon mixes (like 85/15 or 90/10 Ar/CO₂) to give a smoother arc. Stainless wires (ER308LSi and similar) want tri-mix or Ar/O₂, not CO₂-heavy mixes — too much CO₂ carbonises the weld pool and drops corrosion resistance.
Aluminium wire (ER5356, ER4043) wants pure argon below 6mm, and argon/helium blends above. Helium adds heat input, which matters on thick aluminium because aluminium conducts heat away from the weld faster than steel does.
Always read your wire manufacturer’s gas recommendation on the spool. They’ve usually tested it.
- Argon — pure and mixes
- Carbon Dioxide — Industrial
- Oxygen — cutting and brazing support
- Welding application page with the full material spec table.
Call us and we’ll size the cylinder to your actual draw rate — hire cost isn’t worth over-sizing, and under-sizing means mid-shift swaps.